Last updated: 19 November 2026 | Data source:
BASF P3010 TDS.pdfand Eastman Tritan™ TX1001 TDS | Reading time: about 11 minutes
Short answer: PPSU Material is a high-temperature polyphenylsulfone that survives repeated steam sterilization, while Tritan is a clear, BPA-free copolyester built for everyday food-contact parts. Choose PPSU when the part must be boiled or autoclaved repeatedly; choose Tritan when transparency, low weight and cost matter more than heat ceilings.
These two materials are compared constantly in baby bottles, sports bottles, small appliances and reusable medical devices, yet they are not direct competitors. PPSU is a polymer family; Tritan is a trademarked copolyester. This comparison puts the leading grade of each against the other using published supplier data, so the numbers can be checked line by line.
Heat: PPSU deflects at 197 °C under 1.8 MPa; Tritan deflects at 85 °C, a 2.3× gap.
Stiffness: PPSU is about 45 % stiffer (2,250 MPa vs 1,550 MPa tensile modulus).
Transparency: Tritan transmits 90 % of light with haze below 1 %; PPSU is amber-translucent by nature.
Sterilization: PPSU handles superheated steam and autoclave cycles; Tritan is designed for dishwasher exposure, not autoclaving.
Price: PPSU resin typically costs 2.5 to 4 times more than Tritan copolyester.
Safety: Both are BPA-free and food-contact compliant. The real risk is using either outside its temperature window.
Match the requirement to the material before reading the detailed data.
| If your requirement is | Choose | Why |
|---|---|---|
| Baby bottles boiled or steam-sterilized daily | PPSU | Superheated-steam resistance; no deformation across repeated cycles |
| Sports bottles, toddler cups, everyday drinking | Tritan | 90 % light transmission, low weight, roughly half the resin cost |
| Coffee-machine boilers, hot-water valves | PPSU | 197 °C HDT and long-term service near 170–180 °C |
| Reusable medical instruments, autoclave trays | PPSU | Survives 121–134 °C saturated steam |
| Clear cosmetic jars, display containers, blender jugs | Tritan | Glass-like clarity with haze under 1 % |
| Strong alkalis, solvents, aggressive disinfectants | PPSU | Sulfone chemistry outclasses copolyester across the board |
| Precision parts under combined heat, moisture and load | PPSU | Minimal creep; balanced 0.9–1.0 % shrinkage |
The table below uses values exactly as published in the two datasheets. Where a property is not stated by the supplier, it is marked as such rather than estimated.
| Property | PPSU — P3010 | Tritan — TX1001 |
|---|---|---|
| Polymer class | Polyphenylsulfone (PPSU) | Amorphous copolyester (PCTG) |
| Density | 1.285 g/cm3 | 1.18 g/cm3 |
| Glass transition temperature (Tg) | 220 °C (DSC) | Not stated in TDS; PCTG class is far lower |
| Heat deflection temperature, 1.8 MPa | 197 °C | 85 °C |
| Heat deflection temperature, 0.45 MPa | Not stated | 99 °C |
| Tensile modulus | 2,250 MPa | 1,550 MPa |
| Tensile stress at yield | 74 MPa | 43 MPa |
| Elongation at break | Not stated | 210 % (ASTM D638) / 190 % (ISO 527-2) |
| Notched Izod impact, 23 °C | 58 kJ/m2(ISO 180/A) | 93 kJ/m2; (ISO 180) / 980 J/m (ASTM D256) |
| Notched Charpy impact, 23 °C | 70 kJ/m2 | Not stated |
| Notched impact at low temperature | 50 kJ/m2; at -30 °C (Charpy) | 20 kJ/m2; at -40 °C (Izod, ISO 180) |
| Hardness | Ball indentation 124 MPa | Rockwell R112 |
| Light transmission | Amber-translucent | 90 %, haze below 1 % |
| Flammability | UL 94 V-0 at 1.5 mm and 3.0 mm | Not a rated property |
| Molding shrinkage | 0.90 % parallel / 1.00 % normal | 0.50–0.70 % machine direction |
| Water absorption at saturation | 1.2 % | Low (not stated) |
| Coefficient of linear thermal expansion | 55 × 10-6 /K (23–80 °C) | Not stated; higher than PPSU |
| Melt temperature, injection molding | 350–390 °C | 260–282 °C |
| Mold temperature | 140–180 °C | 38–66 °C |
| Predrying before processing | 130–150 °C for at least 4 h | 88 °C for 4–6 h |
| Indicative resin price, 2026 | About 70–220 per kg depending on origin | About 45–75 per kg |
PPSU is a polymer family; Tritan is a brand name. The two belong to different material classes and are only compared because their end uses overlap.
PPSU stands for polyphenylsulfone, a member of the sulfone family alongside polysulfone (PSU) and polyethersulfone (PES). It is an amorphous engineering thermoplastic that is naturally amber-tinted because of its molecular structure. Grades such as BASF Ultrason P3010 are unreinforced, medium-viscosity products for injection molding and extrusion, formulated for toughness, stress-crack resistance and resistance to superheated steam.
Tritan is Eastman Chemical's trademark for a family of amorphous copolyesters, often classified as PCTG. Grade TX1001 is an injection-molding copolyester that includes a vegetable-derived mold release. Its headline properties are clarity, toughness, hydrolytic stability and durability in dishwasher environments.
Reframe the comparison: Tritan's real substitute in the market is polycarbonate, a clear,impact-resistant material that raised BPA concerns. PPSU's true peers are PSU and PES. Pitting PPSU against Tritan means comparing a high-temperature sterilization platform with a clarity-first everyday platform.
PPSU deflects at 197 °C under 1.8 MPa load, more than twice Tritan's 85 °C, and this single difference explains most of the application split between them.
| Thermal metric | PPSU P3010 | Tritan TX1001 |
|---|---|---|
| Glass transition temperature | 220 °C | Not published; substantially lower |
| HDT at 1.8 MPa | 197 °C | 85 °C |
| HDT at 0.45 MPa | Not published | 99 °C |
| Typical long-term service ceiling | 170–180 °C | Around 100 °C in food-contact use |
| Melt processing window | 350–390 °C | 260–282 °C |
The distinction that matters in practice: Tritan's 99 °C deflection at low load means a cup will not collapse when filled with boiling water. It does not mean the part can live at that temperature. PPSU's 197 °C figure describes a continuous load-bearing capability, which is why it appears in boiler components and autoclavable hardware.
PPSU delivers higher stiffness and stable low-temperature toughness, while Tritan delivers much greater elongation and excellent room-temperature impact, but loses impact strength quickly as temperature falls.
At 23 °C, Tritan's notched Izod value of 93 kJ/m2; actually exceeds PPSU's 58 kJ/m2;, and its elongation at break of 210 % is far beyond anything a sulfone will reach. That combination makes Tritan an outstanding drop-resistant material for thin-walled consumer goods.
The picture changes at low temperature. Tritan's notched impact falls to 20 kJ/m2; at -40 °C, while PPSU holds 50 kJ/m2; at -30 °C. PPSU also carries roughly 45 % more tensile modulus and 72 % more yield stress, so it resists deformation under sustained load in a way a copolyester cannot.
Read the two datasheets carefully: they report impact using different methods, PPSU in ISO 180 and ISO 179 units, Tritan in both ASTM D256 and ISO 180. Only the ISO 180 values are directly comparable, and even then specimen geometry differs between suppliers.
PPSU resists strong alkalis, solvents and repeated hot-water exposure that would attack Tritan, making sulfone the safer choice wherever cleaning chemicals or aggressive media are involved.
| Chemical environment | PPSU | Tritan |
|---|---|---|
| Dilute acids and bases | Resistant | Resistant |
| Strong alkalis | Resistant | Not recommended |
| Alcohols | Resistant | Resistant |
| Fats, oils, detergents | Resistant | Resistant |
| Ketones and aromatic hydrocarbons | Partly resistant | Not recommended |
| Long-term hot-water immersion | Hydrolytically stable | Slow aging above about 80 °C |
| Superheated steam | Resistant | Not rated |
Tritan's hydrolytic stability is genuinely good for a copolyester. The TX1001 datasheet explicitly targets the combination of heat, humidity and aggressive detergents found in a dishwasher. What it does not claim is autoclave-grade steam resistance, and prolonged exposure above roughly 80 °C in water tends to produce haze and micro-cracking over time.
PPSU is engineered for superheated steam and repeated autoclave cycles; Tritan is engineered for dishwashers and is not intended for pressurized steam sterilization.
| Method | PPSU | Tritan |
|---|---|---|
| Boiling water, 100 °C | Repeatedly | Occasional; repeated boiling degrades appearance |
| Saturated steam, 121–134 °C | Repeated cycles | Not supported |
| Microwave steam sterilization | Suitable | Suitable with temperature control |
| UV sterilizer cabinet | Suitable | Suitable; gradual yellowing under long UV exposure |
| Dishwasher, normal cycle | Suitable | A design target of the grade |
| Medical autoclave | Standard use | Not applicable |
On cycle counts, be precise about the source. The P3010 datasheet states resistance to superheated steam but does not publish a cycle number. Suppliers of PPSU grades commonly cite figures in the range of 1,000 steam sterilization cycles at 132–134 °C with retained toughness. Treat such figures as supplier test data for that specific grade, not as a generic PPSU guarantee.
Practical rule: Tritan is not unsafe to disinfect. It simply has a temperature ceiling.Steam above 100 °C is outside its design window; boiling water is a short-term contact, not a service condition.
PPSU holds dimensions far better under combined heat, moisture and load, which is why it is chosen for precision and load-bearing parts while Tritan is chosen for appearance parts.
| Factor | PPSU | Tritan |
|---|---|---|
| Molding shrinkage | 0.90 % parallel, 1.00 % normal, near-isotropic | 0.50–0.70 % machine direction |
| Water absorption, saturated | 1.2 % | Low, not published |
| Water absorption, 23 °C / 50 % RH | 0.6 % | Low, not published |
| Thermal expansion, 23–80 °C | 55 × 10-6 /K | Higher than PPSU |
| Creep under load above 100 °C | Minimal | Significant |
| Drying before processing | 130–150 °C, minimum 4 h | 88 °C, 4–6 h |
The near-balanced shrinkage of PPSU is a real manufacturing advantage for parts that must stay round or flat. The trade-off is that PPSU pellets absorb moisture very rapidly. The datasheet is explicit that pellets must be dried at 130–150 °C for at least four hours before processing. Skipping or shortening this step is the most common cause of silver streaks, bubbles and strength loss in PPSU molding.
PPSU covers roughly -40 °C to 180 °C in continuous service with steam, chemicals and UV in play; Tritan covers -40 °C to about 100 °C and is best kept to ambient and warm conditions.
For Tritan, the most common real-world failure mode is not impact or chemical attack, it is thermal. A bottle left in a pot of boiling water, a cup run through a high-temperature steam sterilizer, or a container repeatedly microwaved with a dry load will deform, cloud or yellow well before it breaks.
PPSU dominates applications that must survive heat and repeated sterilization; Tritan dominates applications where clarity, weight and cost drive the decision.
Baby bottles and drinking cups used with daily boiling or steam sterilization
Reusable medical instruments, dental trays, sterilization cassettes
Coffee-machine boiler parts, hot-water valves, filter housings
Laboratory ware and autoclavable containers
Aircraft interior components and high-temperature electrical insulation
Parts requiring a UL 94 V-0 flame rating at 1.5 mm
Sports bottles, toddler cups, shaker and blender jugs
Food storage containers and dry-goods canisters
Clear appliance housings, water tanks, cosmetic jars
Baby products used in low-frequency or non-steam cleaning routines
Transparent retail display packaging
Both materials are BPA-free and suitable for food contact; the meaningful safety question is whether the part stays inside its declared temperature window.
Tritan TX1001 is documented in its own datasheet as suitable for repeated-use food-contact articles under US FDA regulations. It also carries NSF/ANSI Standard 51 certification for food equipment materials and NSF/ANSI Standard 61 certification for drinking-water system components, the latter being a genuinely differentiating credential for water-contact parts.
PPSU grades are widely used in food-contact and medical applications, and many carry FDA, EU 10/2011 and USP Class VI documentation. The P3010 datasheet reviewed here does not itself list FDA clauses, so for any regulated project the compliance statement must be requested per grade and per production site rather than assumed from the polymer type.
Note on bisphenols: Both PPSU and Tritan are marketed as BPA-free, and neither releases bisphenol A under normal use. Bisphenol S has been added to the REACH candidate list of substances of very high concern, so buyers exporting to the EU should request an explicit written declaration covering BPA, BPS and BPF, not just BPA.
PPSU resin costs roughly 2.5 to 4 times more than Tritan copolyester, and the gap widens in finished goods because PPSU also molds at higher temperature with tighter process windows.
| Material | Origin | Indicative price, 2026 |
|---|---|---|
| PPSU | Domestic Chinese producers | about 11–15 USD per kg |
| PPSU | BASF Ultrason, Solvay Radel | about 17–36 USD per kg, medical grades higher |
| Tritan | Eastman TX / MX / FX / EX series | about 6.4–11 USD per kg |
| "Tritan-type" copolyester | Unbranded PCTG | about 4.2–7.4 USD per kg |
These ranges are indicative market pricing, not datasheet values, and move with order volume, grade and exchange rates. On a finished-product basis the gap is partly offset by PPSU's narrower processing window, higher energy consumption and lower molding yield.
Ask about sterilization first, clarity second, and load plus chemistry third. The first yes decides the material.
Must the part be boiled or steam-sterilized repeatedly? If yes, specify PPSU. There is no copolyester substitute.
Is high clarity, low weight or cost the priority? If yes, specify Tritan, provided the temperature ceiling is respected.
Does the part carry sustained load, sit in aggressive chemistry, or require tight dimensional control? If yes, specify PPSU. If not, Tritan or polypropylene at lower cost will usually do the job.
Specify the grade, not the material name, and demand traceable documentation. Counterfeit and blended material is the single largest risk in both supply chains.
Source from traceable grades: Solvay Radel, BASF Ultrason, or established domestic producers
Guard against regrind blending, which is visually hard to detect; request a certificate of analysis per lot
Collect: supplier TDS, FDA 21 CFR statement, EU 10/2011 declaration, food-contact conformity statement
Confirm an Eastman-authorized grade; unbranded "Tritan-type" PCTG is widespread
Collect: supplier TDS, brand authorization, written declaration on BPA, BPS and BPF
Verify the declared maximum use temperature against your actual cleaning routine
Gasket and seal materials, silicone or TPE grade
Printing inks and surface coatings
Assembly adhesives
Whether every wetted component meets the same food-contact standard as the body
It depends on how often you sterilize. For daily boiling or steam sterilization, PPSU is the correct choice because it withstands superheated steam without deformation. If you sterilize occasionally and value transparency and lower cost, Tritan is a reasonable option, but it should not go into a steam sterilizer rated above 100 °C.
Yes, briefly. Tritan TX1001 has a heat deflection temperature of 99 °C at 0.45 MPa, so a short pour of boiling water will not collapse the part. What it cannot tolerate is prolonged contact with boiling water or repeated steam exposure, which causes deformation, clouding and yellowing over time.
At room temperature Tritan is excellent. Its notched Izod impact of 93 kJ/m2; on ISO 180 actually exceeds PPSU's 58 kJ/m2;. But Tritan's impact strength drops to 20 kJ/m2; at -40 °C, while PPSU retains 50 kJ/m2; at -30 °C. PPSU is also roughly 45 % stiffer, so it resists sustained load far better.
The color comes from the polymer backbone. The sulfone linkage in PPSU produces an inherent amber tint that cannot be fully removed, giving roughly 70–85 % light transmission in thin walls. Tritan copolyester transmits 90 % of light with haze below 1 %, which is why it reads as glass-like.
Neither material releases bisphenol A under normal conditions of use, and both are marketed as BPA-free. PPSU is built from bisphenol-type monomers but the finished polymer contains no residual BPA at relevant levels. Tritan is manufactured without BPA. For regulated markets, request a written declaration that also covers BPS and BPF.
PPSU is significantly more expensive. Resin pricing sits around 11–15 USD per kg for PPSU depending on origin, against about 4.2–7.4USD per kg for Tritan, a factor of 2.5 to 4. In finished goods the difference usually widens to 3–5 times because of processing cost.
Yes. Dishwasher durability under heat, humidity and detergent attack is one of the design targets of the TX1001 grade. A dishwasher cycle is not, however, a substitute for autoclave sterilization.
Drying. PPSU pellets absorb moisture very quickly and the datasheet requires 130–150 °C for at least four hours before processing. Add a 350–390 °C melt temperature and a 140–180 °C mold temperature, and the process window is narrow enough that equipment and tooling must be specified for it from the start.
BASF Ultrason®P3010 NAT product technical datasheet, PPSU, 2026 edition
Eastman TritanTM TX1001 product technical datasheet, copolyester
UL Solutions yellow card data for Ultrason P3010
Market pricing ranges compiled from public industry quotations, indicative only
All physical property values above are taken from the supplier datasheets named. Values vary with grade and test method. Confirm against the latest TDS and compliance documents from the supplier before final specification.
PPSU vs Tritan: Heat Resistance, Strength, Chemical Resistance, Price & Sterilization ComparedLast updated: 19 November 2026 | Data source: BASF Ultrason® P3010 TDS and Eastman Tritan™ TX1001 TDS | Reading time: about 11 minutesShort answer: PPSU is a high-temperature polyphenylsulfone that surviv
ItemPPSPPSUChemical StructureBenzene ring + thioether bond -[C6H4-S]-nBiphenyl + sulfone group + ether bondCrystallinitySemi-crystalline (crystallinity 35–50%)AmorphousAppearanceOpaque (off-white/gray/black)Amber, translucentInherent Flame RetardancyUL94 V-0UL94 V-0Water AbsorptionExtremely low ~0.0
Ultra-high flow PEEK is more suitable for micro injection molding machines and high-precision products. PEEK with good fluidity requires less injection pressure and can better fill complex-shaped cavities.
DING Haoliang, TANG Wei, WEI Sai, LI Fan, ZHAO Yunfeng. Development of Bearing Bracket Made From Polyether Ketone by Shot Glass Fiber Reinforced. Aerospace Materials & Technology, 2018, 48(5): 73-77.